Lost circulation is one of the most expensive problems in drilling. When drilling fluid escapes into fractures, or highly permeable rock, crews lose costly mud, rig time, and in the worst cases well control. Lost circulation materials (LCM) are added to the fluid to plug those loss zones. Whether they work depends largely on one thing: whether the particles are the right size and shape for the openings they need to seal.
In this lab session, we put real LCM samples through our Raptor dynamic imaging system using dry powder dispersion. The goal was to see how much more information you get from imaging every particle than from a single size number.
Why LCM Particle Size Matters
Bridging: the right size for the opening
LCM works by bridging. Particles lodge at the mouth of a fracture or pore throat and build a framework, and finer particles then fill the gaps in that framework to form a low-permeability seal. That only happens if the particle size is matched to the opening:
- Too fine: particles flow straight into the fracture or formation without bridging. The fluid loss continues, and the fines can damage the producing zone.
- Too coarse: particles can’t enter the opening to form a bridge. They may also plug downhole tools, bit nozzles, or MWD equipment, or be screened out at the shale shakers before they ever reach the loss zone.
- Correctly sized: a distribution with enough bridging particles near the opening size, plus enough fines to fill the voids, forms a seal quickly and holds it.
That’s why the industry designs LCM blends around particle size distribution, not just around material type.
Rules of thumb engineers use
Several well-established sizing guidelines tie LCM particle size directly to the size of the loss zone:
- Abrams’ rule: the median particle size of the bridging material should be at least one-third of the median pore throat size of the formation.
- Ideal packing theory: the blend’s cumulative size distribution should follow a square-root relationship with particle diameter, which gives the tightest packing and the lowest-permeability seal.
- Fracture-width guidelines: for fractured formations, common practice is to match the blend’s D50 or D90 to the estimated fracture width.
Every one of these rules assumes you know the real particle size distribution of the LCM. If the measurement is wrong, the blend design is wrong too.
Size changes in the field
LCM doesn’t stay the size it was when it left the bag. Particles break down through shear in pumps and bit nozzles, coarse material is stripped out by solids control equipment, and the remaining blend shifts over time. Measuring the LCM in reconditioned mud, not just the fresh product, tells field engineers how much material to add back to maintain the required concentration.
Why shape matters as much as size
LCM includes granular, flaky, and fibrous materials, and they bridge differently. Fibers and elongated particles tend to mat across an opening, granular particles fill and pack, and flakes lie flat against the fracture face. Traditional methods struggle with these shapes:
- Laser diffraction treats every particle as a sphere, so long fibers and flat flakes get reported as an equivalent sphere that doesn’t match how they actually behave.
- Sieve analysis lets elongated particles pass through lengthwise, which underreports their true length.
Dynamic image analysis measures each particle’s actual dimensions and shape, so you can see what fraction of the blend is fibrous, granular, or flaky. For more on this, see why particle shape matters in lost circulation materials.
Testing LCM Samples with the Dry Powder System
The LCM samples for this test were provided by the team at OHS Resources. We had previously analyzed these same samples with wet dispersion. For this run we switched to a dry dispersion configuration to see how the system handles large, coarse particles in their natural, as-supplied state. Coarse, irregular samples like these can be run on the Raptor’s standard dry dispersion or on our recirculating dry powder module, which is useful when sample is limited or particles are fragile.
From Sample Loading to Real-Time Analysis
Results appeared live as the sample ran, and the number-weighted and volume-weighted distributions told two very different stories:
- Number-weighted distribution: dominated by fine particles, with a peak around 20 µm. By count, most of the sample is small.
- Volume-weighted distribution: dominated by coarse particles well beyond 1,000 µm, approaching 2,500 µm. By mass, most of the sample is large.
Both views matter for LCM. The coarse fraction does the bridging, and the fine fraction fills the voids and completes the seal. A single averaged size value would hide one of the two populations, and a blend can only be judged properly when you can see both.
Going Beyond the Numbers: Interactive Particle Classification
After the run, we used the Raptor software to sort the measured particles into classes based on size and shape.
Custom Classifications
| Class | Definition | Result |
|---|---|---|
| Large | 500 – 2,500 µm | Mostly elongated particles |
| Small | Under 500 µm | 61.7% of the particle population |
| Long | Aspect ratio greater than 3:1 | Fibrous or elongated particles |
| Rough | High edge complexity or perimeter variation | Irregular, textured particles |
Classes like these line up directly with how LCM behaves in the well. The large, elongated class is the bridging fraction, the small class is the filler, and the long and rough classes show how much of the blend is fibrous or irregular.
Thumbnail Navigation
The run captured more than 7,000 particle images. Instead of scrolling through all of them, you can click any class and see only the particles in it. That makes it quick to confirm what the “long” or “rough” particles actually look like, spot contaminants or foreign material, and compare blends side by side.
Watch the Full Demonstration
The video walks through this dry powder run, from sample loading to live results and particle classification.
Final Thoughts: Why It Matters
Getting LCM size right is the difference between a fracture that seals and fluid that keeps disappearing downhole. Dynamic image analysis gives drilling fluid engineers the full picture: the real size distribution by count and by volume, the shape of every particle, and images they can check with their own eyes. Those same capabilities carry over to other fields where coarse, irregular particles matter, including additive manufacturing and general quality control.
For a broader look at particle analysis across drilling fluids and barite, see elevating drilling efficiency with advanced particle size and shape analysis.
Special thanks to OHS Resources and Peter Osborne for supplying the samples used in this study.
Test Your Own LCM or Drilling Fluid Samples
Want to see how your LCM blend or reconditioned mud measures up? Talk to our applications team about a sample analysis, or see the Raptor Oil and Gas Edition, which covers drilling mud from 1 to 300 µm and LCM from 20 to 2,500 µm, in both wet and dry modes.